Fatigue strength: PH1 steel (Vxx/ST1)

This page presents the S-N curves and fatigue limit of PH1 steel samples that underwent shot-peening, heat treatment and machining that removed allowance of 1mm (in that order), obtained using the bending tests of rotating bars with AM layers normal to the axis of rotation.

Production and prost-processing conditions

Build orientation of longitudinal axis vertical
Position with respect to inert gas flow undefined
Post-processing shot-peening → heat treatment → machining allowance 1mm

Experimental S-N curve

Experimental method ISO1143, rotating bending test R=-1
AM layers normal to axis of rotation

Wöhler curve

Fatigue limit (MPa) 510
Number of cycles to failure N N=8,55⋅1077⋅S-26,32
Stress amplitude S (MPa) S=915⋅N-0,038

Explanation of the terms are given at the page Fatigue strength description.

This page is a part of the section DMLS/SLM: Fatigue design rules.