This page presents the S-N curves and fatigue limit of MS1 steel samples that underwent shot-peening, heat treatment and machining that removed allowance of 0.5mm (in that order), obtained using the bending tests of rotating bars with AM layers parallel to the axis of rotation.
Build orientation of longitudinal axis | horizontal |
---|---|
Position with respect to inert gas flow | undefined |
Post-processing | shot-peening → heat treatment → machining allowance 0.5mm |
Fatigue limit (MPa) | 595 |
---|---|
Number of cycles to failure N | N=2,30⋅1024⋅S-6,25 |
Stress amplitude S (MPa) | S=7904⋅N-0,16 |
Explanation of the terms are given at the page Fatigue strength description.