This page presents the S-N curves and fatigue limit of CX steel samples that underwent shot-peening, heat treatment and machining that removed allowance of 0.5mm (in that order),), obtained using the bending tests of rotating bars with AM layers normal to the axis of rotation.
| Build orientation of longitudinal axis | vertical |
|---|---|
| Position with respect to inert gas flow | undefined |
| Post-processing | shot-peening → heat treatment → machining allowance 0.5mm |
| Fatigue limit (MPa) | 428 |
|---|---|
| Number of cycles to failure N | N=1,04⋅10<html>21</html>⋅S<html>-5,56</html> |
| Stress amplitude S (MPa) | S=6064⋅N<html>-0,18</html> |
Explanation of the terms are given at the page Fatigue strength description.
This page is a part of the section DMLS/SLM: Fatigue design rules.